Alloy Composition:
Element | % |
Carbon: | 0.94% |
Manganese: | 1.20% |
Silicon: | 0.50% |
Chromium: | 0.50% |
Nickel | 0.30% |
Tungsten: | 0.50% |
Vanadium: | 0.30% |
Copper: | 0.25% |
Phosphorus: | 0.03% |
Sulphur: | 0.03% |
Recommended Heat Treatment
- Coat in ATP-641 Anti Scale Compound.
- Heat and Austenitise at 800?C and hold for 10 minutes.
- Quench in Houghton’s G Medium Quench Oil or a high flash point vegetable oil such as canola or rice bran oil.
- Temper at 175 – 225?C for 2 hours, twice.
Recommended working hardness 56-62HRC.